Complete Set of CAMPUS® Data, ASTM Data, Biopolymer Database, Application Database, Tradename Database, Literature Database, Toolbox.

Material datasheets available free. Online registration at: www.materialdatacenter.com

Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of Ultramid® A3EG7 FC Aqua UN - PA66-GF35 - BASF

Material Data Center offers the following functions for Ultramid® A3EG7 FC Aqua UN:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, parameters for material models, CAE Interfaces

Check here, which other Ultramid A datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
Testo del prodotto
Ultramid® A3EG7FC Aqua UN is optimized for plastic parts, mandatory requiring material approvals for drinking water or direct food contact.
The product is approved according to
• 21 CFR FDA § 177.1500 "Nylon resins". (for repeated use applications only)
• European Food Contact European Food Contact Commission Regulation (EU) 10/2011
• GMP (EC) n°2023/2006

and provides the approvals for drinking water regulations of
• KTW
• DVGW W270
• WRAS
• ACS (disclosure of ingredients)
• NSF (disclosure of ingredients)

For questions regarding the compliance with further regulations, and certificates, please contact your local BASF representative or Plastics Safety (E-Mail: plastics.safety@basf.com).
Caratteristiche Fisichesecco/condUnitáNorma del test
ISO Data
Indice di fusione di volume, MVR 35 / * cm³/10min ISO 1133
Temperatura 275 / * °C -
Carico 5 / * kg -
Ritiro di stampaggio, parallelo 0.5 / * % ISO 294-4, 2577
Ritiro di stampaggio, perpendicolare 1.0 / * % ISO 294-4, 2577
Temperatura di estrazione 195 °C -
Proprietà Meccanichesecco/condUnitáNorma del test
ISO Data
Modulo a trazione 11500 / 8500 MPa ISO 527
Carico unitario a rottura 210 / 150 MPa ISO 527
Deformazione a rottura 3 / 5 % ISO 527
Modulo di scorrimento a trazione, 1000h * / 6650 MPa ISO 899-1
Resistenza all'urto Charpy, +23°C 95 / 105 kJ/m² ISO 179/1eU
Resistenza all'urto Charpy, -30°C 75 / - kJ/m² ISO 179/1eU
Resistenzia all'urto Charpy con intaglio, +23°C 14 / 22 kJ/m² ISO 179/1eA
Resistenzia all'urto Charpy con intaglio, -30°C 12 / - kJ/m² ISO 179/1eA
Resistenza all'urto Izod con intaglio, +23°C 14 / 18 kJ/m² ISO 180/1A
Proprietà Termichesecco/condUnitáNorma del test
ISO Data
Temperatura di fusione, 10°C/min 260 / * °C ISO 11357-1/-3
Temp.di inflessione sotto carico, 1.80 MPa 250 / * °C ISO 75-1/-2
Temp.di inflessione sotto carico, 0.45 MPa 250 / * °C ISO 75-1/-2
Temp.di rammollimento Vicat, B 250 / * °C ISO 306
Coeff.di dilatazione termica lin., parallelo 22 / * E-6/K ISO 11359-1/-2
Coeff.di dilatazione termica lin., perpend. 93 / * E-6/K ISO 11359-1/-2
Reaz. al fuoco spess.nom. 1.5mm HB / * class IEC 60695-11-10
Spessore provato 1.6 / * mm -
Yellow Card disponibile sì / * - -
Reazione al fuoco a spessore h HB / * class IEC 60695-11-10
Spessore provato 0.8 / * mm -
Yellow Card disponibile sì / * - -
Indice di ossigeno 24 / * % ISO 4589-1/-2
Proprietà Elettrichesecco/condUnitáNorma del test
ISO Data
Costante dielettrica relativa, 1MHz 3.5 / 5.7 - IEC 62631-2-1
Fattore di dissipazione, 100Hz 200 / 3000 E-4 IEC 62631-2-1
Fattore di dissipazione, 1MHz 200 / 1500 E-4 IEC 62631-2-1
Resistività volumica >1E13 / 1E11 Ohm*m IEC 62631-3-1
Resistività superficiale * / 1E10 Ohm IEC 62631-3-2
Rigidità dielettrica 40 / 37 kV/mm IEC 60243-1
Res. Alle correnti striscianti superficiali - / 550 - IEC 60112
Altre Proprietàsecco/condUnitáNorma del test
Assorbimento d'acqua 5 / * % Sim. alla ISO 62
Assorbimento d'umidità 1.6 / * % Sim. alla ISO 62
Massa volumica 1410 / - kg/m³ ISO 1183
Bulk density 700 kg/m³ -
Proprietà Specifiche Materialesecco/condUnitáNorma del test
ISO Data
Numero di viscosità 145 / * cm³/g ISO 307, 1157, 1628
Preparazione ProvetteValoreUnitáNorma del test
ISO Data
Stamp. ad Iniezione, temp. di fusione 290 °C ISO 294
Stamp. ad Iniezione, temperatura dello stampo 80 °C ISO 294
Stamp. ad Iniezione, velocità media d'iniezione 200 mm/s ISO 294
Raccomandazione de Processabilità Stampaggio ad IniezioneValoreUnitáNorma del test
Pre-essiccamento - Temperatura 80 °C -
Pre-essiccamento - Tempo 4 h -
Umidità del Processo ≤0.15 % -
Temperatura di fusione 280 - 300 °C -
Temperatura dello stampo 80 - 90 °C -
Funzioni
Viscosità-Velocità di taglio , Ultramid® A3EG7 FC Aqua UN, PA66-GF35, BASF
Sforzo di taglio-Velocità di taglio , Ultramid® A3EG7 FC Aqua UN, PA66-GF35, BASF
Modulo dinamico a taglio-temperatura , Ultramid® A3EG7 FC Aqua UN (Secco), PA66-GF35, BASF
Modulo dinamico a taglio-temperatura , Ultramid® A3EG7 FC Aqua UN (cond.), PA66-GF35, BASF
Sforzi-deformazione , Ultramid® A3EG7 FC Aqua UN (Secco), PA66-GF35, BASF
Sforzi-deformazione , Ultramid® A3EG7 FC Aqua UN (cond.), PA66-GF35, BASF
Modulo secante-deformazione , Ultramid® A3EG7 FC Aqua UN (Secco), PA66-GF35, BASF
Modulo secante-deformazione , Ultramid® A3EG7 FC Aqua UN (cond.), PA66-GF35, BASF
Sforzi-deformazioni (isocrona) 23°C, Ultramid® A3EG7 FC Aqua UN (cond.), PA66-GF35, BASF
Modulo di scorrimento-tempo 23°C, Ultramid® A3EG7 FC Aqua UN (cond.), PA66-GF35, BASF
Curva di scorrimento 23°C, Ultramid® A3EG7 FC Aqua UN (cond.), PA66-GF35, BASF
Sforzi-deformazioni (isocrona) 60°C, Ultramid® A3EG7 FC Aqua UN (Secco), PA66-GF35, BASF
Modulo di scorrimento-tempo 60°C, Ultramid® A3EG7 FC Aqua UN (Secco), PA66-GF35, BASF
Curva di scorrimento 60°C, Ultramid® A3EG7 FC Aqua UN (Secco), PA66-GF35, BASF
Sforzi-deformazioni (isocrona) 90°C, Ultramid® A3EG7 FC Aqua UN (Secco), PA66-GF35, BASF
Modulo di scorrimento-tempo 90°C, Ultramid® A3EG7 FC Aqua UN (Secco), PA66-GF35, BASF
Curva di scorrimento 90°C, Ultramid® A3EG7 FC Aqua UN (Secco), PA66-GF35, BASF
Sforzi-deformazioni (isocrona) 120°C, Ultramid® A3EG7 FC Aqua UN (Secco), PA66-GF35, BASF
Modulo di scorrimento-tempo 120°C, Ultramid® A3EG7 FC Aqua UN (Secco), PA66-GF35, BASF
Curva di scorrimento 120°C, Ultramid® A3EG7 FC Aqua UN (Secco), PA66-GF35, BASF
Sforzi-deformazioni (isocrona) 140°C, Ultramid® A3EG7 FC Aqua UN (Secco), PA66-GF35, BASF
Modulo di scorrimento-tempo 140°C, Ultramid® A3EG7 FC Aqua UN (Secco), PA66-GF35, BASF
Curva di scorrimento 140°C, Ultramid® A3EG7 FC Aqua UN (Secco), PA66-GF35, BASF
Volume specifico-temperatura (pvT) , Ultramid® A3EG7 FC Aqua UN, PA66-GF35, BASF
Modulo a taglio-temperatura , Ultramid® A3EG7 FC Aqua UN (Secco), PA66-GF35, BASF
Modulo a taglio-temperatura , Ultramid® A3EG7 FC Aqua UN (cond.), PA66-GF35, BASF
Caratteristiche
Processabilità e Forma di Forni
Stampaggio ad Iniezione, Altre Estrusioni
Forma fisica disponibile
Pellet, Colore naturale
Additivi
Lubrificanti, Agente di distacco
Caratteristiche speciali
Stabilizzato o stabile al calore
Certifications
Contatto con gli alimenti, Approvato per l'utilizzo per contatto con alimenti 10/2011, Approvato per l'utilizzo per contatto con alimenti secondo la FDA 21 CFR, Contatto con acqua potabile, Contacto con acqua potabile KTW, Contatto con acqua potabile DVGW W270, Contatto con acqua potabile NSF 61
Applicazioni
Automotive
Disponibilità geografica
Altre informazioni
Stampaggio ad Iniezione
PREPROCESSING
Pre/Post-processing, max. allowed water content: .15 %
Pre/Post-processing, Pre-drying, Temperature: 80 °C
Pre/Post-processing, Pre-drying, Time: 4 h

PROCESSING
injection molding, Melt temperature, range: 280 - 300 °C
injection molding, Melt temperature, recommended: 290 °C
injection molding, Mold temperature, range: 80 - 90 °C
injection molding, Mold temperature, recommended: 80 °C
injection molding, Dwell time, thermoplastics: 10 min
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.